Just finished a test by immersing a test piece of aluminium in some of our fine California 5% ethanol auto gas. Left it there for 2 months. There were some very fine white spots spread around the surface, just barely visible. About like you would expect if left exposed to air. May have been on original sample, have to check source lot. Pretty much zip damage. Sanded off one side to remove any posssible protective cladding. Put back in for another month. Three months total. No additional corrosion on unsanded side. Zero corrosion on "exposed" sanded side.
So much for that little tidbit of generic knowledge.
Think I will do hoses next.
DC
So much for that little tidbit of generic knowledge.
Think I will do hoses next.
DC
Comment